化工社化工社 化学情報印刷レポート · 研究参考用
epsilon-CAPROLACTONE → epsilon-Caprolactone p-Dioxanone
関与物質
| 役割 | 名称 | HCID | 仕込み量 |
|---|---|---|---|
| 反応物 | epsilon-CAPROLACTONE | HCID 10401 | — |
| 反応物 | Dioxanone | HCID 18233 | — |
| 生成物 | epsilon-Caprolactone p-Dioxanone | HCID 86748302 | — |
反応手順
The procedure in Example 5A is substantially repeated except that 45.7 grams (0.40 mole) of ε-caprolactone and 61.3 grams (0.60 mole) of p-dioxanone were used. The copolymer was dried under vacuum (0.1 mm Hg) at 80° C. for about 80 hours to remove any unreacted monomer. The copolymer had an inherent viscosity of 0.18 dL/g in HFIP at 25° C. The copolymer was a liquid at room temperature. The molar ratio of PCL/PDS was found to be 46.7/53.3 by proton NMR.
情報源と証拠
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|---|
| 特許番号 | US05728752 |
| 出典データセット | uspto-grants-1998_03 |
| ORD ID | ord-38955b7c995840b4ae3dced0500d7938 |
| 出典メモ | uspto-grants-1998_03 |