[C:1]([O:5][CH2:6][CH2:7][CH2:8][CH2:9][CH2:10][CH:11]([CH3:13])[CH3:12])(=[O:4])[CH:2]=[CH2:3].[C:14]([OH:18])(=[O:17])[CH:15]=[CH2:16].C(O)(C)C>C(OCC)(=O)C>[C:1]([O:5][CH2:6][CH2:7][CH2:8][CH2:9][CH2:10][CH:11]([CH3:13])[CH3:12])(=[O:4])[CH:2]=[CH2:3].[C:14]([OH:18])(=[O:17])[CH:15]=[CH2:16]Isooctyl acrylate (173.9 g), acrylic acid (11.1 g) azobisisobutyronitrile (0.37 g), ethyl acetate (313.425 g) and isopropanol (1.575 g) were placed in a 1 quart (946 mL) bottle. The mixture was deoxygenated by purging with nitrogen (1L/min) for 2 minutes. The bottle was sealed and placed in a 55° C. rotating water bath for 24 hours to effect essentially complete polymerization. The inherent viscosity in ethyl acetate was 0.97 deciliter/gram.