HuagongsheHuagongshe Chemie-Druckbericht · Nur für Forschungszwecke
Ammonia → Acrylamide-acrylic acid resin
Beteiligte Stoffe
| Rolle | Name | HCID | Einwaage |
|---|---|---|---|
| Edukt | Ammonia | HCID 222 | — |
| Edukt | Acrylamide | HCID 6579 | — |
| Edukt | Acrylic Acid | HCID 6581 | — |
| Lösungsmittel | Water | HCID 962 | — |
| Produkt | Acrylamide-acrylic acid resin | HCID 62693 | — |
Reaktionsschritte
To a stainless steel beaker was charged 214 g. of glacial acrylic acid (Rohm and Haas Production Grade). While stirring with a magnetic stirrer, 29% aqueous ammonia (technical) was added and the temperature was maintained at ≤35° C. until the pH became 7.5 (about 1.5 hours). Distilled water was added to bring the total weight to 428 g. The solution was transferred to a 1 liter glass beaker and while stirring 1.07 g. of methone was added (0.5% based on the acrylic acid). It dissolved in about 10 minutes. Then 23 g. of 50% acrylamide was added and the procedure of Examples 29-38 was followed to emulsion polymerize the monomers.
Herkunft & Nachweise
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|---|
| Patentnummer | US04568731 |
| Quelldatensatz | uspto-grants-1986_02 |
| ORD ID | ord-9f5b74bbd6364ac683a742da4d0ffb71 |
| Quellennotiz | uspto-grants-1986_02 |