Beteiligte Stoffe
| Rolle | Name | HCID | Einwaage |
|---|
| Edukt | Acrylamide | HCID 6579 | — |
| Edukt | Acrylic Acid | HCID 6581 | — |
| Lösungsmittel | Water | HCID 962 | — |
| Produkt | Acrylamide-acrylic acid resin | HCID 62693 | — |
Reaktionsschritte
56 grams 50% acrylamide, 12 grams acrylic acid and 127 grams water were mixed, and warmed up to 30° C. Nitrogen was used to purge the flask. Then 0.7 gram ammonium persulfate in 3 grams of water and 0.7 gram sodium metabisulfite in 3 grams water were added, respectively. After 20 minutes, the reaction began to take place, the temperature slowly rose to 78° C. (max.) after stirring for 1.5 hour a 20% copolymer was thus produced with an acrylamide/acrylic acid ratio of 70/30. 7 grams NaOH in 30 grams water was then added to neutralize the copolymer.
Herkunft & Nachweise
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patentnummer | US04515855 |
|---|
| Quelldatensatz | uspto-grants-1985_05 |
|---|
| ORD ID | ord-afb2cfbf8f8b4735958f3371f9372578 |
|---|
| Quellennotiz | uspto-grants-1985_05 |
|---|