Beteiligte Stoffe
| Rolle | Name | HCID | Einwaage |
|---|
| Edukt | Aluminum Stearate | HCID 12496 | — |
| Edukt | Lithium Stearate | HCID 517357 | — |
| Produkt | Ethylene brassylate | HCID 61014 | 88,9% |
Reaktionsschritte
A mixed metal catalyst comprised of aluminum stearate and lithium stearate (molar ratio 1:1) was used for the depolymerization. For the reaction aluminum stearate (1.09 gram) and lithium stearate (0.36 gram) were blended in 70 grams poly(ethylene brassylate) at 200° C. The temperature was then raised to 314° C. while maintaining a vacuum of 0.05-0.1 mm Hg. Ethylene brassylate was obtained (40 mls during the first hour) in an 88.9 percent yield. Of the ethylene brassylate recovered, 90 percent of the product was obtained after 2 hours.
Herkunft & Nachweise
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patentnummer | US04499288 |
|---|
| Quelldatensatz | uspto-grants-1985_02 |
|---|
| ORD ID | ord-0f676f5a41704569b949cc4c945350ba |
|---|
| Quellennotiz | uspto-grants-1985_02 |
|---|