[C:1](S(O[Li])=O)([C:4](C(C(C([C:16]([C:19]([C:22]([F:25])([F:24])[F:23])(F)[F:20])([F:18])[F:17])(F)F)(F)F)(F)F)(F)F)([F:3])[F:2]>O>[F:23][C:22]([F:25])([F:24])[C:19]([F:20])=[C:16]([F:18])[F:17].[C:1]([F:3])([F:2])=[CH2:4]A 400 ml autoclave was loaded with 200 ml water, 1.09 g of C8F17SO2Li, and purged with nitrogen. The autoclave was cooled, evacuated, and loaded with 60 g of hexafluoropropylene and 40 g of vinylidene fluoride. A solution of 0.5 g of sodium bromate in 50 ml of water was injected at 0.3 ml/minute. Pressure within the autoclave decreased from 2.15 MPa at 22° C. to 1.65 MPa at 24° C., 3 hours later. The autoclave was vented, the polymeric emulsion recovered and then broken by freezing. Filtering and drying gave 38 g of hexafluoropropylene/vinylidene fluoride copolymer with an inherent viscosity of 0.37.