関与物質
| 役割 | 名称 | HCID | 仕込み量 |
|---|
| 反応物 | 2,2-Dimethylhexane | HCID 11551 | — |
| 溶媒 | Carbon Tetrachloride | HCID 5943 | — |
| 生成物 | 2-Methylbuta-1,3-diene--2-methylprop-1-ene (1/1) | HCID 62703 | — |
反応手順
A 3.5% solution of 10 g of poly(isobutylene-co-isoprene) was prepared in 96.5% of a 1:1 mixture of trimethylpentane and CCl4. The solution was purged with N2, heated to 75° C., 0.3 g of benzoyl peroxide was added, followed by 40 g of methylmethacrylate, added over a period of 1 hour. The polymerization was carried out for 16 hours with constant mechanical stirring. After cooling to room temperature, the cleaning procedure used was identical to that of Example 1.
情報源と証拠
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 特許番号 | US04644041 |
|---|
| 出典データセット | uspto-grants-1987_02 |
|---|
| ORD ID | ord-d951b2b78e8b4edf9165641b535f0515 |
|---|
| 出典メモ | uspto-grants-1987_02 |
|---|