反応式
[CH:1]#[C:2][C:3]1[CH:8]=[CH:7][C:6]([OH:9])=[CH:5][CH:4]=1.[C:10]([O:13][CH:14]([CH3:18])[CH2:15]OC)(=[O:12])[CH3:11]>>[CH:3]1([CH2:2][CH2:1][O:12][CH:10]([O:13][C:14]2[CH:15]=[CH:8][C:3]([CH:2]=[CH2:1])=[CH:4][CH:18]=2)[CH3:11])[CH2:8][CH2:7][CH2:6][CH2:5][CH2:4]1.[OH:9][C:6]1[CH:7]=[CH:8][C:3]([CH:2]=[CH2:1])=[CH:4][CH:5]=1参加物
反応条件
- 温度
- 20 °C
実験手順
In 320 g of propylene glycol monomethyl ether acetate (PGMEA) was dissolved 70 g of poly(p-hydroxystyrene) (VP-8000, manufactured by Nippon Soda Co., Ltd.) with heating and the solution was subjected to dehydration by distillation under a reduce pressure and cooled to 20° C. To the solution were added 0.35 g of pyridinium p-toluenesulfonate and 22.4 g of 2-cyclohexylethanol. Then, 17.5 g of tert-butyl vinyl ether was gradually added to the solution, followed by reacting at 20° C. for 5 hours. To the reaction mixture were added 0.28 g of triethylamine and 320 ml of ethyl acetate and the mixture was washed three times with each 150 ml of distilled water. The solvent was distilled off to concentrate, the resulting oily substance was dissolved in 100 ml of acetone and the solution was gradually poured into 2 liters of distilled water. The powder thus-deposited was collected by filtration and dried to obtain 54 g of the desired compound. The Mw of the resin was 12,000 and the molecular weight distribution (Mw/Mn) thereof was 1.1.
後処理
- temperaturewith heating
- distillationthe solution was subjected to dehydration by distillation under a reduce pressure
- additionTo the solution were added 0.35 g of pyridinium p-toluenesulfonate and 22.4 g of 2-cyclohexylethanol
- additionThen, 17.5 g of tert-butyl vinyl ether was gradually added to the solution
- additionTo the reaction mixture were added 0.28 g of triethylamine and 320 ml of ethyl acetate
- washthe mixture was washed three times with each 150 ml of distilled water
- distillationThe solvent was distilled off
- concentrationto concentrate
- dissolutionthe resulting oily substance was dissolved in 100 ml of acetone
- additionthe solution was gradually poured into 2 liters of distilled water
- filtrationThe powder thus-deposited was collected by filtration
- customdried
出典と根拠
- ORDレコード
- ord-c34343c0dabe40fc82375b76a7b8d25f
- 出典データセット
- uspto-grants-2004_06
- 特許番号
- US06756179B2
関連ノート
読み込み中…