戻る
化工社化工社 化学情報印刷レポート · 研究参考用
HRID 379495作成日:2026年10月26日

Glycolic Acid → Poliglecaprone

https://huagongshe.com/reaction/379495

反応式

関与物質

役割名称HCID仕込み量
反応物Glycolic AcidHCID 757—
反応物2-ethylhexanoic acid tin(II) saltHCID 9318—
反応物epsilon-CAPROLACTONEHCID 10401—
反応物GlycolideHCID 65432—
生成物PoliglecaproneHCID 65431—

反応条件

温度150 °C

反応手順

Glycolide (0.21 moles) was mixed with ε-caprolactone (4.0 moles) and a catalytic amount of stannous octoate (0.8 mole) and glycolic acid (0.40 moles). The system was heated to 150° C. and was stirred at this temperature for 14 hours. At the conclusion of the reaction, the unreacted monomer was removed by heating at 120° C. under reduced pressure for 1 hour. The resulting polymer had a peak melting temperature of 54.3° C. as measured by DSC.

情報源と証拠

DOI10.6084/m9.figshare.5104873.v1
特許番号US06299631B1
出典データセットuspto-grants-2001_10
ORD IDord-515a6a6c9ec040f88ec84ca01eb6da11
出典メモuspto-grants-2001_10