ホームMCPワークベンチSkills
ホームワークベンチ通知マイページ
llms.txt · MCPガイドプライバシーポリシー · 利用規約 · サポートv1.8.3
  1. ホーム
  2. /反応

Vinyl Acetate → Butyl acrylate vinyl acetate

HRID 487795
印刷

反応式

HRID 487795 の反応式
S(OOS([O-])(=O)=O)([O-])(=O)=O.[K+].[K+].[C:13]([O:16][CH:17]=[CH2:18])(=[O:15])[CH3:14].[C:19]([O:23][CH2:24][CH2:25][CH2:26][CH3:27])(=[O:22])[CH:20]=[CH2:21].S(O)O.C=O>O>[C:13]([O:16][CH:17]=[CH2:18])(=[O:15])[CH3:14].[C:19]([O:23][CH2:24][CH2:25][CH2:26][CH3:27])(=[O:22])[CH:20]=[CH2:21]
参加物反応条件実験手順後処理出典と根拠反応ノート

参加物

6

反応物 4

HCID 7904Vinyl AcetateHCID 8846Butyl AcrylateHCID 24412Potassium PersulfateHCID 21967118Formaldehyde sulfoxylate

生成物 1

HCID 23373234Butyl acrylate vinyl acetate

試薬・触媒・溶媒 1

HCID 962Water溶媒

反応条件

温度
80 °C

実験手順

A vinyl acetate-butyl acrylate copolymer was prepared utilizing the sulfonate product of Example 5 as the sole surfactant. A one liter resin kettle was charged with a solution of 31.7 grams of the sulfonate product of Example 5 in 281 grams of deionized water. The solution was heated to 80° C. under a nitrogen atmosphere. One gram of potassium persulfate (K2S2O8) was added to the solution followed by the slow addition of 50 milliliters of a mixture comprising 202 grams of vinyl acetate and 36 grams of butyl acrylate. The polymerization temperature was maintained at 75°-80° C. for 30 minutes after the addition of the 50 milliliter portion of the monomer mixture. The remainder of the monomer mixture was charged to the kettle over a 3-4 hour period while maintaining the polymerization temperature at between 70° C. and 75° C. The contents of the resin kettle were post stirred at 70° C. for 1 hour and then 10 grams of 2 percent formaldehyde sulfoxylate added to the kettle to complete the polymerization.

後処理

  1. temperatureThe polymerization temperature was maintained at 75°-80° C. for 30 minutes
  2. additionafter the addition of the 50 milliliter portion of the monomer mixture
  3. additionThe remainder of the monomer mixture was charged to the kettle over a 3-4 hour period
  4. temperaturewhile maintaining the polymerization temperature at between 70° C. and 75° C
  5. customthe polymerization

出典と根拠

ORDレコード
ord-173ea3ec6c1f4b4ab97d524dd2bb5b91
出典データセット
uspto-grants-1994_03
DOI
10.6084/m9.figshare.5104873.v1
特許番号
US05296627

反応ノート

このページの内容参加物反応条件実験手順後処理出典と根拠反応ノート