反応式
[C:1]([O:4][CH:5]=[CH2:6])(=[O:3])[CH3:2].[C:7]1(=[O:13])[O:12][C:10](=[O:11])[CH:9]=[CH:8]1.C(OOC(=O)CCCCCCCCCCC)(=O)CCCCCCCCCCC>C1C=CC=CC=1>[C:1]([O:4][CH:5]=[CH2:6])(=[O:3])[CH3:2].[C:10]1(=[O:11])[O:12][C:7](=[O:13])[CH:8]=[CH:9]1参加物
5
反応条件
- 温度
- 70 °C
実験手順
13 g (0.5 mole) of vinyl acetate, 49 g (0.5 mole) of maleic acid anhydride and 0.1 g of lauroyl peroxide were dissolved in 400 cc of benzene and heated for five hours at 70° C. The copolymer was precipitated from the viscous solution with petroleum ether (80° to 100° C.). The copolymer dissolved well in diluted caustic soda.
後処理
- customThe copolymer was precipitated from the viscous solution with petroleum ether (80° to 100° C.)
- dissolutionThe copolymer dissolved well in diluted caustic soda
出典と根拠
- ORDレコード
- ord-a8ca235c9ca844d4bdd9af51edf5e228
- 出典データセット
- uspto-grants-1987_06
- 特許番号
- US04671982