関与物質
| 役割 | 名称 | HCID | 仕込み量 |
|---|
| 反応物 | Adipic Acid | HCID 196 | — |
| 反応物 | 4-Methoxyphenol | HCID 9015 | — |
| 反応物 | 2-Hydroxyethyl acrylate | HCID 13165 | — |
| 反応物 | Neopentyl glycol | HCID 31344 | — |
| 反応物 | 2,6-Di-tert-butyl-4-methylphenol | HCID 31404 | — |
| 反応物 | Isocyanate | HCID 105034 | — |
| 反応物 | Isophorone diisocyanate | HCID 169132 | — |
| 反応物 | Cesium acetate | HCID 5152919 | — |
| 溶媒 | Ethanol | HCID 702 | — |
| 生成物 | Urethane acrylate | HCID 21863578 | — |
反応手順
672.0 g of a polyester of adipic acid and neopentyl glycol with an OH number of about 200, 140.0 g of hydroxyethyl acrylate, 0.6 g of hydroquinone monomethyl ether, 1.21 g of 2,6-di-tert-butyl-4-methylphenol, 0.12 g of cesium acetate were initially introduced into a round-bottomed flask and heated to 50° C. 400.0 g of isophorone diisocyanate were then added dropwise over the course of 30 minutes. The mixture was left to react for a further 7 hours at 90-95° C., during which the NCO content dropped to 0.56%. The mixture was cooled to 60° C., then 520.0 g of ethanol were added and the mixture was left to react further for about 2 hours at 65-70° C. until the isocyanate content (NCO value) had dropped to 0. The resulting resin was filtered over a 50 μm filter and bottled.
情報源と証拠
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 特許番号 | US08821841B2 |
|---|
| 出典データセット | uspto-grants-2014_09 |
|---|
| ORD ID | ord-e11022da67c7404caadfbb5793860415 |
|---|
| 出典メモ | uspto-grants-2014_09 |
|---|