関与物質
| 役割 | 名称 | HCID | 仕込み量 |
|---|
| 反応物 | Ethanol | HCID 702 | — |
| 反応物 | N-vinyl-2-pyrrolidone | HCID 6917 | — |
| 反応物 | Vinyl Acetate | HCID 7904 | — |
| 反応物 | Sodium Hydroxide | HCID 14798 | — |
| 溶媒 | Diethyl Ether | HCID 3283 | — |
| 生成物 | Ganex E 535 | HCID 270885 | 95% |
反応手順
Into a 2 liter round bottom flask 800 ml of ethanol, 12.8 g of sodium hydroxide pellets and 80 g of a copolymer composed of 70% N-vinylpyrrolidone and 30% vinyl acetate are introduced. The resulting reaction mixture is maintained with stirring at 30° C. for 2 hours and is then poured into 8 liters of diethyl ether to precipitate the desired polymer. After filtration the polymer is dried under reduced pressure. Yield: 95%.
情報源と証拠
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 特許番号 | US04283384 |
|---|
| 出典データセット | uspto-grants-1981_08 |
|---|
| ORD ID | ord-89a3e98d71a44dd59f10265f058e1e6b |
|---|
| 出典メモ | uspto-grants-1981_08 |
|---|