참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|
| 반응물 | Aluminum Stearate | HCID 12496 | — |
| 반응물 | Lithium Stearate | HCID 517357 | — |
| 생성물 | Ethylene brassylate | HCID 61014 | 88.9% |
반응 단계
A mixed metal catalyst comprised of aluminum stearate and lithium stearate (molar ratio 1:1) was used for the depolymerization. For the reaction aluminum stearate (1.09 g) and lithium stearate (0.36 g) were blended in 70 g poly(ethylene brassylate) at 200° C. The temperature was then raised to 314° C. while maintaining a vacuum of 0.05-0.1 mm Hg. Ethylene brassylate was obtained (40 mls during the first hour) in an 88.9% yield. Of the ethylene brassylate recovered, 90% of the product was obtained after 2 hours.
출처 및 근거
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 특허 번호 | US04393223 |
|---|
| 출처 데이터셋 | uspto-grants-1983_07 |
|---|
| ORD ID | ord-87f4e281078c4305b7525009f18c66b4 |
|---|
| 출처 메모 | uspto-grants-1983_07 |
|---|