Etidronic Acid → ZINC oxide ZINC etidronate
참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|---|---|---|
| 반응물 | Etidronic Acid | HCID 3305 | — |
| 반응물 | Zinc Oxide | HCID 3007857 | — |
| 생성물 | ZINC oxide ZINC etidronate | HCID 131716685 | — |
반응 단계
First, 1030 g of a solution of etidronic acid (206 g as etidronic acid) was heated to 70° C. and 2035 g of a zinc oxide slurry (407 g as zinc oxide) held at 70° C. was added dropwise over about 2 hours with stirring. The mol ratio of zinc oxide to etidronic acid was 5/1. This slurry was stirred at 60° to 70° C. for 5 hours and, then, cooled to room temperature. The slurry was filtered and the dehydrated cake was washed with distilled water 3 to 5 times and, then, subjected to dehydration, drying and pulverization to give a zinc oxide/zinc etidronate composition.