[C:1]([O:5][CH2:6][CH3:7])(=[O:4])[CH:2]=[CH2:3].[C:8](#[N:11])[CH:9]=[CH2:10].[C:12]([OH:16])(=[O:15])[CH:13]=[CH2:14].C(S)CCCCCCCCCCC.C(OOCCCCCCCCCCCC)CCCCCCCCCCC.C(OOC(=O)C1C=CC=CC=1)CCC>C1(C)C(C)=CC=CC=1>[CH2:6]([O:5][C:1](=[O:4])[CH:2]=[CH2:3])[CH3:7].[C:12]([OH:16])(=[O:15])[CH:13]=[CH2:14].[C:8](#[N:11])[CH:9]=[CH2:10]참가 물질
8
실험 절차
this polymer material was produced by adding to 320g xylene at 100° C. the monomer solution and a catalyst solution over a period of 3 hours. The monomer solution contained 2.900g ethyl acrylate, 76g acrylonitrile, 76g acrylic acid and 3g laurylmercaptan. The catalyst solution contained 26g laurylperoxide and 7g butylperbenzoate in 273g of xylene. The material was highly viscous with comonomer proportions of 95:2.5:2.5.