Huagongshe화공사 화학 정보 인쇄 보고서 · 연구 참고용
Sodium Phosphate, Dibasic → Hydroxylapatite (Ca5(OH)(PO4)3)
참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|---|---|---|
| 반응물 | Sodium Phosphate, Dibasic | HCID 24203 | — |
| 반응물 | Calcium Chloride | HCID 5284359 | — |
| 생성물 | Hydroxylapatite (Ca5(OH)(PO4)3) | HCID 14781 | — |
반응 단계
Brushite was prepared in the same manner as in Example 1 except that 1 l of an aqueous calcium chloride solution of 0.5 mol/l in concentration and 1 l of an aqueous disodium phosphate solution of 0.5 mol/l in concentration were used and reaction temperature was room temperature. Then, at 95° C., 300 ml of an aqueous sodium hydroxide solution of 1 mol/l in concentration was added to the resulting brushite over a period of 1 hour to obtain hydroxylapatite in the form of platy crystal [hereinafter referred to as "hydroxylapatite (H)"].
출처 및 근거
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|---|
| 특허 번호 | US05073357 |
| 출처 데이터셋 | uspto-grants-1991_12 |
| ORD ID | ord-3664f7782a164eccb7ae4d550227b3ea |
| 출처 메모 | uspto-grants-1991_12 |