반응식
[CH:1]([O:3][CH3:4])=[CH2:2].[C:5]1(=[O:11])[O:10][C:8](=[O:9])[CH:7]=[CH:6]1>O>[CH:1]([O:3][CH3:4])=[CH2:2].[C:5]([OH:10])(=[O:11])/[CH:6]=[CH:7]\[C:8]([OH:3])=[O:9]참가 물질
5
실험 절차
Copoly(methyl vinyl ether:maleic anhydride)(50:50) (Grantrez AN-119 available from GAF)(20.6 grams) was suspended in 80 grams of water and heated on a steam bath to form a 20% solids clear solution of copoly(methyl vinyl ether:maleic acid) (50:50) in water. To 61.8 grams of the solution (containing 12.4 grams of copolymer and 8.26 grams (0.072 mole) of maleic acid)) was added 4.0 grams (0.072 mole) of potassium hydroxide in order to half-neutralize all maleic acid present. Glycerol (9.3 grams) was also added as a plasticizer. The impedance of a bioelectrode prepared with the material was 33 Kohms.
후처리
- temperatureheated on a steam bath
출처 및 근거
- ORD 기록
- ord-3aae0e6382004311ad259d73daea250a
- 출처 데이터셋
- uspto-grants-1982_10
- 특허 번호
- US04352359
연결된 노트