참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|
| 반응물 | Vinyl Chloride | HCID 6338 | — |
| 반응물 | Trichloroethylene | HCID 6575 | — |
| 반응물 | Lauroyl peroxide | HCID 7773 | — |
| 반응물 | Vinyl Acetate | HCID 7904 | — |
| 용매 | Water | HCID 962 | — |
| 생성물 | Vinyl chloride-vinyl acetate | HCID 61927 | — |
반응 단계
An aqueous slurry of a vinyl chloride/vinyl acetate copolymer was prepared by heating in an autoclave at 65° C. for 18 hours a polymerization system that contained 85 parts of vinyl chloride, 15 parts of vinyl acetate, 185 parts of deionized water, 0.125 part of dilauroyl peroxide, 1.75 parts of gelatin, and 0.69 part of trichloroethylene. The slurry was heated under vacuum at a temperature below 65° C. to reduce its vinyl chloride content to less than 5000 ppm.
출처 및 근거
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| 특허 번호 | US04150219 |
|---|
| 출처 데이터셋 | uspto-grants-1979_04 |
|---|
| ORD ID | ord-4609186026ef46f584cdf2d746a0082d |
|---|
| 출처 메모 | uspto-grants-1979_04 |
|---|