Sodium Hydroxide → Sodium orthosilicate
참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|---|---|---|
| 반응물 | Sodium Hydroxide | HCID 14798 | — |
| 반응물 | Sodium Silicate | HCID 23266 | — |
| 생성물 | Sodium orthosilicate | HCID 26051 | — |
반응 단계
(Comparison) 1600 kg of water glass with an SiO2/Na2O ratio of 2.06 and an active substance content of 45.5% were admixed with 36.8 kg of sodium hydroxide solution (48% strength) and spray-dried in a spray tower from Kestner to give an amorphous sodium silicate having an active substance content of 83%. 15 kg of the amorphous sodium silicate are heat-treated at 720° C. for 90 min in a muffle furnace (Nabertherm, model W1000/H). A second batch is treated identically. The chilled materials (about 24 kg) are pulverized using a jaw crusher and a disk mill.