Glycolic Acid → Poliglecaprone

https://huagongshe.com/reaction/379495

반응식

참여 물질

역할이름HCID투입량
반응물Glycolic AcidHCID 757—
반응물2-ethylhexanoic acid tin(II) saltHCID 9318—
반응물epsilon-CAPROLACTONEHCID 10401—
반응물GlycolideHCID 65432—
생성물PoliglecaproneHCID 65431—

반응 조건

온도150 °C

반응 단계

Glycolide (0.21 moles) was mixed with ε-caprolactone (4.0 moles) and a catalytic amount of stannous octoate (0.8 mole) and glycolic acid (0.40 moles). The system was heated to 150° C. and was stirred at this temperature for 14 hours. At the conclusion of the reaction, the unreacted monomer was removed by heating at 120° C. under reduced pressure for 1 hour. The resulting polymer had a peak melting temperature of 54.3° C. as measured by DSC.

출처 및 근거

DOI10.6084/m9.figshare.5104873.v1
특허 번호US06299631B1
출처 데이터셋uspto-grants-2001_10
ORD IDord-515a6a6c9ec040f88ec84ca01eb6da11
출처 메모uspto-grants-2001_10