Azobisisobutyronitrile → Vinylpyrrolidone lauryl methacrylate
참여 물질
| 역할 | 이름 | HCID | 투입량 |
|---|---|---|---|
| 반응물 | Azobisisobutyronitrile | HCID 6547 | — |
| 반응물 | N-vinyl-2-pyrrolidone | HCID 6917 | — |
| 반응물 | Lauryl Methacrylate | HCID 8906 | — |
| 생성물 | Vinylpyrrolidone lauryl methacrylate | HCID 20459467 | — |
반응 단계
The N-vinyl-2-pyrrolidone/lauryl methacrylate (6/94) copolymer was prepared in the following manner. In 100 parts of 0-grade Solvent L were placed 47 parts of lauryl methacrylate, 3 parts of N-vinyl-2-pyrrolidone and 0.2 parts of azobisisobutyronitrile (polymerization initiator). The mixture was reacted at 60 to 70° C. for about 12 hours at nitrogen atmosphere.
출처 및 근거
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|---|
| 특허 번호 | US05998075 |
| 출처 데이터셋 | uspto-grants-1999_12 |
| ORD ID | ord-48795fde0e514c28afb9751c2a4e4355 |
| 출처 메모 | uspto-grants-1999_12 |