Aluminum Stearate → Ethylene brassylate

https://huagongshe.com/reaction/615479

반응식

참여 물질

역할이름HCID투입량
반응물Aluminum StearateHCID 12496—
반응물Lithium StearateHCID 517357—
생성물Ethylene brassylateHCID 6101488.9%

반응 조건

온도314 °C

반응 단계

A mixed metal catalyst comprised of aluminum stearate and lithium stearate (molar ratio 1:1) was used for the depolymerization. For the reaction aluminum stearate (1.09 gram) and lithium stearate (0.36 gram) were blended in 70 grams poly(ethylene brassylate) at 200° C. The temperature was then raised to 314° C. while maintaining a vacuum of 0.05-0.1 mm Hg. Ethylene brassylate was obtained (40 mls during the first hour) in an 88.9 percent yield. Of the ethylene brassylate recovered, 90 percent of the product was obtained after 2 hours.