Benzoyl Peroxide → 2-Propenoic acid, butyl ester, polymer with diethenylbenzene and ethenylbenzene

HRID 1034120Notes

Reaction equation

HRID 1034120 reaction equation
[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[C:9]([O:13][CH2:14][CH2:15][CH2:16][CH3:17])(=[O:12])[CH:10]=[CH2:11].[C:18](OOC(=O)C1C=CC=CC=1)(=O)[C:19]1C=CC=CC=1>C(C(C)=O)C(C)C>[CH3:17][CH2:16][CH2:15][CH2:14][O:13][C:9]([CH:10]=[CH2:11])=[O:12].[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.[CH2:1]=[CH:2][C:3]1[C:8]([CH:18]=[CH2:19])=[CH:7][CH:6]=[CH:5][CH:4]=1

Participants

5

Conditions

Temperature
90 °C

Procedure

40 parts by weight of methyl isobutyl ketone were put into a flask with a stirrer, and heated to 90° C. with stirring in a stream of nitrogen gas. A mixture of 95 parts by weight of styrene, 10 parts by weight of butyl acrylate and 25 parts by weight of benzoyl peroxide was added dropwise over a period of 6 hours to the methyl isobutyl ketone which was maintained at 90° C. Subsequently, the above-mentioned mixture was subjected to polymerization at 90° C. for 10 hours, whereby a styrene-butyl acrylate copolymer solution was obtained.

Workup

  1. temperaturewas maintained at 90° C
  2. customSubsequently, the above-mentioned mixture was subjected to polymerization at 90° C. for 10 hours

Sources & evidence

ORD record
ord-5d8aaddb63b9412e9b85c33f884ca599
Source dataset
uspto-grants-1994_05
Patent number
US05314777

Reaction notes

Loading…