Participants
| Role | Name | HCID | Charge |
|---|
| Reactant | Nitrogen | HCID 947 | — |
| Reactant | Vinyl Acetate | HCID 7904 | — |
| Reactant | Butyl vinyl ether | HCID 8108 | — |
| Reactant | Sodium Hydroxide | HCID 14798 | — |
| Solvent | Methanol | HCID 887 | — |
| Solvent | Water | HCID 962 | — |
| Product | HCID 86742155 | HCID 86742155 | 381.4% |
Reaction Steps
172.2 g (2.00 moles) of vinyl acetate, 15.1 g (0.15 mole) of n-butyl vinyl ether, 56.2 g of methanol and 0.28 g of 2,2'-azobis-2,4-dimethylvaleronitrile were mixed and polymerized in an atmosphere of N2 at 62° C. for 8 hours. Subsequently, 749.2 g of 5% water-containing methanol and 8.0 g (0.20 mole) of caustic soda were added to the reaction product for saponification at 45° C. for 2 hours. The reaction mixture was milled and filtered to obtain a polymer portion, followed by washing with 5% water-containing alcohol to eliminate impurities such as sodium acetate therefrom. The purified polymer was dried under reduced pressure and milled to obtain 82.5 g of a white powdery vinyl alcohol/n-butyl vinyl ether (93/7 by molar ratio) copolymer (hereinafter referred to as PVA/n-BVE).
Provenance & Evidence
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patent number | US04743441 |
|---|
| Source dataset | uspto-grants-1988_05 |
|---|
| ORD ID | ord-c85e05ed7fc643568293170c76f5793c |
|---|
| Source note | uspto-grants-1988_05 |
|---|