Participants
| Role | Name | HCID | Charge |
|---|
| Reactant | Nitrate | HCID 943 | — |
| Reactant | Sodium Carbonate | HCID 10340 | — |
| Reactant | Cupric nitrate | HCID 18616 | — |
| Reactant | Zinc | HCID 23994 | — |
| Reactant | Zinc Nitrate | HCID 24518 | — |
| Solvent | Water | HCID 962 | — |
| Product | Copper carbonate | HCID 14452 | — |
| Product | Zinc Carbonate | HCID 19005 | — |
Reaction Steps
Each of the mixtures of copper nitrate and zinc nitrate at a Zn/(Zn+Cu) atomic ratio of 0.1, 0.2, 0.3, 0.5 and 0.67, respectively, was dissolved in an ionexchanged water at a concentration of 20 wt %. Separately, a 20 wt % aqueous solution containing a stoichiometric amount of sodium carbonate was prepared. The resulting sodium carbonate solution was added dropwise to the solution of nitrate mixture while stirring in a stirring tank to produce a precipitate of basic copper carbonate and basic zinc carbonate. The precipitate was filtered, washed with water and dried at 120° C. for 10 hours. The precipitate was then calcined at a temperature of 350° C. for 5 hours to obtain five mixtures of cupric oxide and zinc oxide having different proportions.
Provenance & Evidence
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patent number | US04743435 |
|---|
| Source dataset | uspto-grants-1988_05 |
|---|
| ORD ID | ord-e725425ce2c24d888156e5c8220f9d95 |
|---|
| Source note | uspto-grants-1988_05 |
|---|