HRID129358
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
PROCEDURE
实验过程
Hydroxylapatite in an amount of 1.0 kg is added to 10 liters of water together with 32 g of silver nitrate and 69 g of zinc nitrate, and then the whole was stirred to make a reaction. The solids are separated off to form a cake, then the cake is rinsed thoroughly with distilled water and dried. The washed cake is heated or fired at 1200° C. and powdered to provide the antibacterial hydroxylapatite carrying about 2% by weight of silver in a metallic state and 1.5% by weight of zinc in a metallic state.
WORKUP
后处理
- customa reaction
- customThe solids are separated off
- customto form a cake
- washthe cake is rinsed thoroughly with distilled water
- customdried
- temperatureThe washed cake is heated
- customfired at 1200° C.