PROCEDURE
实验过程
A reaction vessel containing 53.5 parts of Polyepoxide A (80 percent solids in isophorone) was heated to 70°C. There were added 3 parts of an amine produced by reacting dimethylethanolamine with dodecylsuccinic anhydride, and then there were added 6 parts of a second amine produced from dimethylethanolamine and maleic anhydride. During the second addition the temperature was raised to 95°C. and stirring was continued for 15 minutes at this temperature. The product when diluted with water and electrodeposited, as in the above examples, provided an adherent solvent-resistant coating.