Reaction Conditions
| Temperature | 170 fahrenheit |
|---|
Reaction Steps
To 900 grams of water, while under agitation, was added 180 grams of ethylene diamine, 60 grams of melamine and char and/or phase transfer catalysts as set forth in Table 4 below. The mixture was warmed to 170° F. and, while maintaining temperature, phosphoric acid was slowly added until a pH of 7.0 was reached. The mixture was cooled, filtered, dried and ground to recover the flame retardant.
Provenance & Evidence
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patent number | US06733697B2 |
|---|
| Source dataset | uspto-grants-2004_05 |
|---|
| ORD ID | ord-13e1167855d54067a5a4691608a7ecc0 |
|---|
| Source note | uspto-grants-2004_05 |
|---|