HRID1603400
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
PROCEDURE
实验过程
The material was prepared by dispersing 0.80 g Tergitol TMN-06 in 1481 g deionized water with an air mixer. To this was then added 1159 g of ground crystalline silicotitanate (150 g, 13.0% solids) (IONSIV IE 910) with agitation. Slowly to this was added 150.1 g Goodrite 1800×73 (39% solids, 58.5 g) with stirring. This mixture was mixed for 1 hour with an air mixer. The slurry was spray dried using a Niro Atomizer, (Serial number #2402) at 35 mL/min. Spray drying conditions were as follows:
WORKUP
后处理
- customThe material was prepared
- additionThis mixture was mixed for 1 hour with an air mixer
- customdried
- customSpray drying conditions