反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
CONDITIONS
反应条件
- 温度
- 300 fahrenheit
PROCEDURE
实验过程
The following experimental procedure was utilized to test physical properties of nonwoven substrates impregnated with the tetramethylol glycoluril-containing VAE copolymer emulsions. The copolymer binder was applied to the substrate using the Atlas padding technique. The emulsions were initially diluted with deionized water to 9.0% solids and the pH was adjusted to 4.0 with ammonium chloride. Whatman #4 chromatography paper was saturated with the binder, the samples were dried, heated at 300° F. for five minutes and then subjected to tensile testing. The strips were immersed in solvent for three minutes and then placed in an Instron (2" jaw span, 1"/min. crosshead speed) for testing.
WORKUP
后处理
- additioncontaining VAE copolymer emulsions
- customthe samples were dried