In a glass polymerization bottle were charged 80 g isooctyl acrylate (IOA), 18 g isobornyl acrylate (IBA), 2 g vinyldimethylazlactone (VDM), 100 g ethyl acetate, 0.5 g benzoyl peroxide and 0.04 g carbon tetrabromide. The bottle was purged with nitrogen, sealed and tumbled in a water bath maintained at 60° C. for 12 hours to produce a IOA/IBA/VDM terpolymer. The polymer was isolated by precipitation in isopropanol and dried under vacuum.