HRID1855649
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
AUXILIARIES
试剂、催化剂与溶剂
PROCEDURE
实验过程
The catalyst was synthesized using impregnation method. 10 g of the above crushed zirconium oxide (0.85 mm and 1.18 mm) was placed in a round bottom reactor. 0.56 g of tin oxalate and 0.54 g of ammonium oxalate was dissolved in 10 ml of water. 0.3 g of palladium nitrate hydrate, tetraammineplatinum(II) nitrate, was added to the tin oxalate solution, followed by impregnating to the above zirconium oxide by stepwise incipient wetness using a rotating dryer. The metal-coated zirconium oxide was dried and calcined under the conditions in Example 1.
WORKUP
后处理
- customThe catalyst was synthesized
- customwas placed in a round bottom reactor
- dry with materialThe metal-coated zirconium oxide was dried