Water → Benzene, ethenyl-, polymer with 1,3-butadiene

HRID 1879239Notes

Reaction equation

HRID 1879239 reaction equation
[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1.C=CC=C.C([Li])CCC.O>CCCCCC>[CH2:1]=[CH:2][CH:3]=[CH2:4].[CH2:1]=[CH:2][C:3]1[CH:8]=[CH:7][CH:6]=[CH:5][CH:4]=1

Participants

6

Procedure

To a 2-gallon reactor equipped with turbine agitator blades was added 1597 g of hexane, 399 g of 34.0 wt % styrene in hexane, and 2440 g of 22.3 wt % 1,3-butadiene in hexane. To the reactor was charged 2.58 mL of 1.6 M n-butyllithium in hexane and 0.85 mL of 1.6 M 2,2-bis(2′-tetrahydrofuryl)propane in hexane. The batch was heated by applying hot water to the reactor jacket. Once the batch temperature reached 55° C., the reactor jacket was cooled with cold water. Two hours after the addition of the catalyst, the polymer cement was removed from the reactor and coagulated with 3 gallons of isopropanol containing 7 g of 2,6-di-tert-butyl-4-methylphenol, and then drum-dried. The properties of the resulting unmodified SBR are summarized in Table 4.

Workup

  1. customTo a 2-gallon reactor equipped with turbine agitator blades
  2. temperatureThe batch was heated
  3. customreached 55° C.
  4. additionTwo hours after the addition of the catalyst
  5. customthe polymer cement was removed from the reactor
  6. customdrum-dried

Sources & evidence

ORD record
ord-aca517b94fd346f2a86a5a37aeef6d9c