Sodium Hydroxide → Zirconium phosphate
Reaction equation
S([O-])([O-])(=O)=O.[Zr+4:6].S([O-])([O-])(=O)=O.[P:12]([O-:16])([OH:15])([OH:14])=[O:13].[NH4+].[Zr].[P].[OH-].[Na+]>>[P:12]([O-:16])([O-:15])([O-:14])=[O:13].[Zr+4:6].[P:12]([O-:16])([O-:15])([O-:14])=[O:13].[P:12]([O-:16])([O-:15])([O-:14])=[O:13].[P:12]([O-:16])([O-:15])([O-:14])=[O:13].[Zr+4:6].[Zr+4:6]Participants
6
Conditions
- Temperature
- 150 °C
Procedure
An aqueous zirconium sulfate solution and an aqueous ammonium dihydrogenphosphate solution were mixed at a ratio of zirconium and phosphorus of 2:3 to produce a precipitate. Then, pH of the resulting slurry was adjusted to 2 with an aqueous sodium hydroxide solution, followed by heating at 150° C. for 24 hours in the hydrothermal state to obtain crystalline zirconium phosphate.
Workup
- customto produce a precipitate
Sources & evidence
- ORD record
- ord-4529f52341264ac694d0fb4512351e39
- Source dataset
- uspto-grants-1997_12
- Patent number
- US05698229
Reaction notes
Loading…