HRID1952391

反应详情

EQUATION

反应方程式

HRID 1952391 的结构方程式

AUXILIARIES

试剂、催化剂与溶剂

1

CONDITIONS

反应条件

温度
40 °C

PROCEDURE

实验过程

To a 500 mL four-necked flask equipped with magnetic stirrer was charged 250 mL of toluene. The toluene was heated to 34° C. To this was added a toluene solution of 0.043 g (1.6 mmol) of polymethylaluminoxane composition based on aluminum atoms. Bis(n-butylcyclopentadienyl)zirconium dichloride ((nBu-Cp)2ZrCl2) was added to achieve an Al/Zr mole ratio of 5,000. While raising the temperature to 40° C., ethylene gas was blown in. After 10 minutes, the ethylene gas feed was halted and methanol was introduced to deactivate the catalyst. The polyethylene produced was filtered and dried. The polymerization activity was calculated to be 35×106 g-PE/mol-Zr·atm·hr.

WORKUP

后处理

  1. customTo a 500 mL four-necked flask equipped with magnetic stirrer