HuagongsheHuagongshe Chemistry Print Report · For research reference only
Acrylamide → Isooctyl Acrylate Acrylamide Vinyl Acetate
Participants
| Role | Name | HCID | Charge |
|---|---|---|---|
| Reactant | Acrylamide | HCID 6579 | — |
| Reactant | Vinyl Acetate | HCID 7904 | — |
| Reactant | 2,2'-Azobis(2,4-dimethylvaleronitrile) | HCID 91537 | — |
| Reactant | Isooctyl acrylate | HCID 165746 | — |
| Solvent | Methanol | HCID 887 | — |
| Solvent | Ethyl Acetate | HCID 8857 | — |
| Product | Isooctyl Acrylate Acrylamide Vinyl Acetate | HCID 86608178 | — |
Reaction Steps
Isooctyl acrylate (148 g), acrylamide (12 g), vinyl acetate (40 g), 2,2'azobis(2,4-dimethylpentanenitrile) (0.30 g), ethyl acetate (310 g) and methanol (30.7 g) were added to a glass bottle. The bottle was purged with nitrogen for 3 minutes at a flow rate of 1 liter per minute. The bottle was sealed and placed in a rotating water bath at 45° C. for 29.5 hours to effect essentially complete polymerization. The inherent viscosity in ethyl acetate was 1.20 deciliter/g.
Provenance & Evidence
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|---|
| Patent number | US05494680 |
| Source dataset | uspto-grants-1996_02 |
| ORD ID | ord-b5582cea65964209908cad0f61c9fd5a |
| Source note | uspto-grants-1996_02 |