HRID26570

反应详情

EQUATION

反应方程式

HRID 26570 的结构方程式

AUXILIARIES

试剂、催化剂与溶剂

1

CONDITIONS

反应条件

温度
65 °C

PROCEDURE

实验过程

An aqueous slurry of a vinyl chloride/vinyl acetate copolymer was prepared by heating in an autoclave at 65° C. for 18 hours a polymerization system that contained 85 parts of vinyl chloride, 15 parts of vinyl acetate, 185 parts of deionized water, 0.125 part of dilauroyl peroxide, 1.75 parts of gelatin, and 0.69 part of trichloroethylene. The slurry was heated under vacuum at a temperature below 65° C. to reduce its vinyl chloride content to less than 5000 ppm.

WORKUP

后处理

  1. temperatureThe slurry was heated under vacuum at a temperature below 65° C.