The method of the present invention generally involves the mixture of titanium dioxide and hot concentrated phosphoric acid in a reaction vessel. The reaction mixture has a phosphorus pentoxide to titanium dioxide mole ratio greater than one. Preferably, the phosphorus pentoxide to titanium dioxide mole ratio is about 1.06 or more, and most preferably about 1.20 to about 1.25. The reactants are thoroughly mixed and heated at temperatures of about 400° C. to about 500° C. to produce a fine titanium pyrophosphate powder having a significantly higher fines yield over conventional titanium pyrophosphate processes. The fines yield is greater than 90% when using a phosphorus pentoxide to titanium dioxide mole ratio of about 1.20 to about 1.25.
WORKUP
后处理
- additionThe reactants are thoroughly mixed
- temperatureheated at temperatures of about 400° C. to about 500° C.