HRID323846
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
PROCEDURE
实验过程
Same as C5 except that monomer emulsion was composed of 5 g of SDS, 1 g of sodium persulfate, 110 g of ethyl methacrylate, 70 g of n-butyl methacrylate, and 20 g of ethylene glycol dimethacrylate. Glass transition temperature was 60° C., average particle size was 29 nm and % solids was 20.7%.