Same as C5 except that the monomer emulsion was composed of 5 g of SDS, 1 g of sodium persulfate, 90 g of ethyl methacrylate, 90 g of n-butyl methacrylate, 10 g of methacrylic acid, and 10 g of ethylene glycol dimethacrylate. Glass transition temperature was 66° C., average particle size was 38 nm and % solids was 21.1%.