HRID323849
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
PROCEDURE
实验过程
Same as C5 except that the monomer emulsion was composed of 5 g of SDS, 1 g of sodium persulfate, 80 g of ethyl methacrylate, 100 g of n-butyl methacrylate, 10 g of methacrylic acid, and 10 g of ethylene glycol dimethacrylate. Glass transition temperature was 69° C., average final particle size was 39 nm and % solid was 20.9%.