HRID341721
反应详情
EQUATION
反应方程式
REACTANTS
反应物
PRODUCTS
生成物
PROCEDURE
实验过程
Reaction between 500 grams of isophorone diisocyanate and 62.6 grams of cyclohexyl isocyanate was effected in the presence of 5.63 grams of a carbodiimidizing catalyst (3methyl-1-phenyl-2-phospholene-1-oxide) at 180° C. for 24 hours, yielding isophorone carbodiimide having a degree of polymerization of 10. The carbodiimide resin was thoroughly pulverized. To 200 grams of this carbodiimide, 200 grams of distilled water having 1 gram of a nonylphenyl nonionic surfactant (Nonypol) dissolved therein was slowly added, obtaining a carbodiimide dispersion (resin concentration 50% by weight).