Participants
| Role | Name | HCID | Charge |
|---|
| Reactant | Water | HCID 962 | — |
| Reactant | Toluene | HCID 1140 | — |
| Reactant | Epichlorohydrin | HCID 7835 | — |
| Reactant | Sodium Hydroxide | HCID 14798 | — |
| Product | Diglycidyl ether | HCID 16704 | — |
Reaction Steps
100 parts of hydrogenated polyisoprene glycol (PIP-H, average molecular weight of 2500, made by Idemitsu Petrochemicals Corp. Japan), 9 parts of epichlorohydrin, 0.15 part of trifluoroborondiethylether complex and 50 parts of toluene were fed and carried out addition reaction under vigorous stirring at 55 degrees C. for 5 hours in the nitrogen atmosphere. Then, 9.5 parts of 48% aqueous solution of sodium hydroxide were added and a ring-closing reaction was carried out at 65 degrees C. for 5 hours. After the reaction 100 parts of water were added and the following procedures were carried out same as described in Reference Example No. 1 and 95 parts of glycidyl ether of hydrogenated polyisoprene glycol (b) were obtained. The glycidyl ether (b) had an epoxy equivalent weight of 1,430 g/eq.
Provenance & Evidence
| DOI | 10.6084/m9.figshare.5104873.v1 |
|---|
| Patent number | US05162437 |
|---|
| Source dataset | uspto-grants-1992_11 |
|---|
| ORD ID | ord-e45c0aaefed746338f58db9da1860c6e |
|---|
| Source note | uspto-grants-1992_11 |
|---|