In this way, the reaction was conducted for 48 hours while continuously adding the aqueous solution of mixture of nickel nitrate, cobalt nitrate and magnesium nitrate, the aqueous ammonia and the aqueous solution of sodium hydroxide to the reactor. During the reaction, the concentration of ammonia in the reaction mixture (slurry) in the reactor was kept within a range from 1.0 to 1.3 mol/L and the reaction temperature was kept at 30° C.±1° C. with a temperature controller. After the completion of the reaction, the slurry in the reactor was filtered, lashed with water and dried to provide a powder of nickel cobalt magnesium hydroxide.

WORKUP

后处理

  1. additionwhile continuously adding
  2. customDuring the reaction
  3. customwas kept at 30° C.±1° C. with a temperature controller
  4. customAfter the completion of the reaction
  5. filtrationthe slurry in the reactor was filtered
  6. customdried