PROCEDURE
实验过程
24 g of helio fast blue HG (C.I. no. 74160), 6 g of a copolymer formed from 75% of lauryl methacrylate and 25% of isobutyl methacrylate with a molecular weight of 150 000, and 210 g of isododecane are mixed for 10 hours using a bead vibrating mill. 100 g of the dispersion obtained are diluted with 100 g of isododecane and reacted with vigorous stirring over a period of 30 minutes at 25° C. with a mixture of 4.5 g of isobutyl cyanoacrylate and 1.5 g of allyl cyanoacrylate. The dispersion was stirred for a further 2 hours at 25° C., then centrifuged and the isolated solid matter was washed with isododecane, centrifuged again and dried. 30 g of coated blue pigment are obtained.