HRID866313

反应详情

EQUATION

反应方程式

HRID 866313 的结构方程式

PROCEDURE

实验过程

The aqueous copolymer dispersion was prepared in an analogous manner to example 11, but by carrying out the polymerization with a modified monomer mixture at an ethylene pressure of 5 atmospheres. A mixture of 764 g of vinyl acetate and 76 g of monochloroacetic acid vinyl ester was added to the polymerization mixture at room temperature and after the polymerization had started a mixture of 6880 g of vinyl acetate and 688 g of monochloroacetic acid vinyl ester was introduced by pumping over a period of 6 hours. The dispersion obtained of a copolymer of vinyl acetate/monochloroacetic acid vinyl ester/ethylene had a solids content of 51% by weight and a latex viscosity of 23 poises.

WORKUP

后处理

  1. customThe aqueous copolymer dispersion was prepared in an analogous manner to example 11
  2. additionwas added to the polymerization mixture at room temperature
  3. additionwas introduced