O.FC([O:16]C(F)=[C:18]([C:20]([F:29])([F:28])[C:21]([F:27])([F:26])[C:22](F)(F)F)F)=C(F)C(F)(F)C(F)(F)C(F)(F)F.FC(F)=C(F)F>FC1(F)CCC1(F)F>[F:29][C:20]1([F:28])[CH2:18][CH2:22][C:21]1([F:26])[F:27].[OH2:16]A 400-mL pressure vessel was loaded with 100 mL of deionized water. The pressure vessel was then chilled and maintained around -20° C. while further loading with 5 mL of 0.05M HFPO dimer peroxide in 1,1,2,2-tetrafluorocyclobutane, pulling the air off with a vacuum pump, adding 5 g of perfluoropropylvinyl ether, and finally adding 50 g of tetrafluoroethylene. Polymerization set in during warm up, first pressure drop occurring above 20° C. The pressure thereafter dropped, falling to 43 psi three to four hours later at 35° C. The product was washed three times with 200 mL of methanol and once with 200 mL of Freon® 113, filtered, and dried under vacuum, giving 38 g of white powder that analysed for 2.6 weight percent PPVE by IR. Under melt indexer conditions, no melt flow was observed at 372° C. with a 15-kg weight.