Reaktionsgleichung
C(#N)C=C.C=CC1C=CC=CC=1.C(C1C=C[C:19]([OH:22])=[CH:18][CH:17]=1)(C)=C.C[CH:24]([CH2:27][CH:28]([CH3:30])[CH3:29])[C:25]#N.N(C(C)(CC(C)C)C#N)=NC(C)(CC(C)C)C#N>C(OCC)(=O)C>[C:28]([C:27]1[CH:24]=[CH:25][CH:17]=[CH:18][C:19]=1[OH:22])([CH3:29])=[CH2:30]Komponenten
7
Versuchsvorschrift
Acrylonitrile (270 g), styrene (630 g), p-isopropenylphenol (100 g), ethyl acetate (250 g) and 2,2'-azobis(2,4-dimethylvaleronitrile (5 g) were fed and polymerized at 60° C. for 4 hours, followed by further adding ethyl acetate (250 g) and 2,2'-azobis(2,4-dimethylvaleronitrile) (5 g) and further polymerization at 60° C. for 4 hours. Solvent was then removed under reduced pressure to obtain a copolymer of isopropenylphenol (hereinafter abbreviated to phenolic polymer B). The viscosity of 5% solution of phenolic polymer B in ethyl acetate, at 25° C., was 1.75 cps.
Aufarbeitung
- custompolymerized at 60° C. for 4 hours
- additionby further adding
- customSolvent was then removed under reduced pressure
Quellen und Nachweise
- ORD-Eintrag
- ord-4f9eff447c2f4eafac50bafd399301cc
- Quelldatensatz
- uspto-grants-1983_03
- Patentnummer
- US04378450
Verknüpfte Notizen
Wird geladen…