Reaktionsgleichung
[C:1]1(=[O:8])[O:7][CH2:6][CH2:5][CH2:4][CH2:3][CH2:2]1.[C:9]1(=[O:15])[O:14][CH2:13][CH2:12][CH2:11][O:10]1.C(O)CCCCCCCCCCC>>[C:1]1(=[O:8])[O:7][CH2:6][CH2:5][CH2:4][CH2:3][CH2:2]1.[C:9]1(=[O:15])[O:14][CH2:13][CH2:12][CH2:11][O:10]1Komponenten
4
Reaktionsbedingungen
- Temperatur
- 135 °C
Versuchsvorschrift
ε-Caprolactone (40 g, 0.35 mole), trimethylene carbonate (10 g. 0.098 mole), lauryl alcohol (1.42 g, 7.6×10-3 mole) and stannous chloride dihydrate (10.1 mg, 4.5×10-5 mole) were combined in a flask and heated for 24 hours under nitrogen at 135° C. The resulting polymer had an inherent viscosity of 0.42 dl/g (0.5 g/dl in HFAS). The composition was determined by 1H NMR to be 86 wt. % caprolactone and 14 wt. % trimethylene carbonate.
Quellen und Nachweise
- ORD-Eintrag
- ord-f4de669701c24b4e80a2207d144b91af
- Quelldatensatz
- uspto-grants-1988_12
- Patentnummer
- US04791929
Verknüpfte Notizen
Wird geladen…